某核电厂装卸料机气管卷筒发条弹簧在机组大修卸料过程中发生断裂.采用宏观观察、化学成分分析、金相检验、硬度测试、扫描电镜分析等方法对弹簧断裂的原因进行分析.结果表明:弹簧内端的局部退火工艺温度过高,使显微组织转变为片状珠光体+断续网状铁素体,同时产生了严重表面脱碳现象,碳元素含量偏低、硬度大幅下降,材料的力学性能显著劣化;弹簧内端弯钩弯折角处存在应力集中,当工作应力超出该区域材料的承载极限时,该处发生以韧性断裂为主的韧-脆混合断裂.
The winding spring of the gas tube drum of a loading and unloading machine in a nuclear power plant broke during the unloading process of the unit during major maintenance.The cause of spring fracture was analyzed using macroscopic observation,chemical composition analysis,metallographic examination,hardness testing and scanning electron microscopy analysis.The results show that the local annealing process temperature at the inner end of the spring was too high,which caused the microstructure to transform into lamellar pearlite+intermittent network ferrite,while also producing severe surface decarburization,low carbon content,significant decrease in hardness,and significant deterioration of mechanical properties of the material.There was stress concentration at the bending angle of the inner hook of the spring.When the working stress exceeded the material bearing limit in this area,a ductile brittle mixed fracture mainly characterized by ductile fracture occurred at this location.
刘君;徐科;聂振华;王坤
中核运维技术有限公司,杭州 311215中核核电运行管理有限公司,嘉兴 314000苏州热工研究院有限公司,苏州 215004苏州热工研究院有限公司,苏州 215004
通用工业技术
发条弹簧60Si2MnA钢退火工艺脱碳韧性断裂
winding spring60Si2MnA steelannealing processdecarbonizationductile fracture