首页|期刊导航|理化检验-物理分册|核电厂低压氮气系统螺柱开裂原因

核电厂低压氮气系统螺柱开裂原因OA

Causes of stud cracking in the low-pressure nitrogen system of a nuclear power plant

中文摘要英文摘要

某沿海核电厂低压氮气管道法兰A2-70钢双头螺柱光杆段发生脆性开裂问题.采用宏观观察、金相检验、化学成分分析、硬度测试、扫描电镜及能谱分析、点化学及晶间腐蚀试验等方法对螺柱开裂的原因进行分析.结果表明:该螺柱在生产过程中产生了较大冷加工变形,且未开展固溶热处理,导致材料内部碳化物未能充分溶解,并沿晶界呈网状连续析出分布;未经过固溶处理的螺柱耐点蚀性能大幅降低,晶间腐蚀敏感性显著提升.螺柱光杆段与法兰接触面形成了狭小的密闭缝隙,该处积聚雨水并滞留高湿海洋大气,造成了缝隙区域持续腐蚀;在拉应力作用下,螺栓最终发生沿晶应力腐蚀开裂.

A brittle fracture occurred in the smooth rod section of the A2-70 steel stud bolts on the low-pressure nitrogen pipeline flange of a coastal nuclear power plant.The causes of the stud fracture were analyzed using methods such as macroscopic observation,metallographic examination,chemical composition analysis,hardness testing,scanning electron microscopy and energy spectrum analysis,chemical and intergranular corrosion tests.The results show that the stud underwent significant cold working deformation during production and was not subjected to solution heat treatment,which led to insufficient dissolution of internal carbides,which formed a continuous network-like distribution along the grain boundaries.The absence of solution treatment significantly reduced the stud's resistance to pitting corrosion and markedly increased its susceptibility to intergranular corrosion.The narrow and enclosed gap between the smooth rod section of the stud and the flange contact surface accumulated rainwater and remained exposed to high-humidity marine atmosphere,caused continuous corrosion in the gap area.Under the tensile stress experienced during service,the stud ultimately fractured through intergranular stress corrosion.

高腾飞;陈文浩;郭凯;李心刚;罗真;翟新年;侯桂林

大亚湾核电运营管理有限责任公司,深圳 518000苏州热工研究院有限公司,苏州 215000大亚湾核电运营管理有限责任公司,深圳 518000大亚湾核电运营管理有限责任公司,深圳 518000中核凯利深圳核能服务股份有限公司,深圳 518000中核凯利深圳核能服务股份有限公司,深圳 518000中核凯利深圳核能服务股份有限公司,深圳 518000

通用工业技术

螺柱固溶热处理碳化物沿晶应力腐蚀开裂电化学试验

studsolution heat treatmentcarbideintergranular stress corrosion crackingelectrochemical testing

《理化检验-物理分册》 2026 (8)

45-49,5

10.11973/lhjy-wl260183

评论