某核电站主蒸汽系统疏水器下游至冷凝器的疏水管道发生壁厚减薄.采用宏观观察、化学成分分析、金相检验、硬度测试、扫描电镜及能谱分析等方法对疏水管道减薄的原因进行分析.结果表明:该疏水管道因疏水器前后压降显著,下游压力长期低于饱和蒸汽压,疏水管道出口高速气液两相流冲刷管壁,产生了闪蒸冲蚀现象,导致管道壁厚减薄;管道管径偏小、焊趾引发局部湍流、疏水器泄漏等问题导致气液两相流持续冲刷,进一步加剧了管道壁厚减薄现象.

The wall thickness of the condensate hydrophobic pipeline downstream of the steam separator to the condenser in a nuclear power plant's main steam system was thinned.Macroscopic observation,chemical composition analysis,metallographic inspection,hardness testing,scanning electron microscopy and energy spectrum analysis were employed to analyze the cause of the pipe thinning.The results show that the thinning was caused by flashing erosion due to high-speed gas-liquid two-phase flow at the pipe outlet,resulting from significant pressure drop across the steam separator and prolonged downstream pressure below the saturated steam pressure.Additionally,issues such as small pipe diameter,turbulent flow induced by weld toes,and steam separator leakage led to continuous gas-liquid two-phase flow erosion,further exacerbating the pipe wall thinning.

陈子航;张舟永;陈新

苏州热工研究院有限公司 材料工程技术中心,苏州 215004苏州热工研究院有限公司 材料工程技术中心,苏州 215004苏州热工研究院有限公司 材料工程技术中心,苏州 215004

通用工业技术

疏水管道闪蒸冲蚀壁厚减薄气液两相流压降

hydrophobic pipelineflash erosionwall thickness thinninggas-liquid two-phase flowpressure drop