某核电厂辅助给水泵在大修解体时导叶发生断裂.采用宏观观察、扫描电镜及能谱分析、化学成分分析、金相检验、力学性能测试、有限元分析等方法对导叶断裂的原因进行分析.结果表明:叶片侧面过渡拐角存在铸造工艺遗留的耐火材料夹杂缺陷,破坏了基体表面的连续性并产生应力集中;在交变流体运行载荷与结构振动激振力耦合的作用下,缺陷位置萌生疲劳裂纹,裂纹持续扩展,最终导致导叶发生疲劳断裂.

During the overhaul and disassembly of the auxiliary feedwater pump at a nuclear power plant,it was discovered that the guide vane fractured.The causes of guide vane fracture were analyzed using macroscopic observation,scanning electron microscopy and energy spectrum analysis,chemical composition analysis,metallographic examination,mechanical property testing,finite element analysis.The results show that there were refractory material inclusions left over from the casting process at the transition corners of the blade side,which damaged the continuity of the substrate surface and caused stress concentration.Under the coupling effect of alternating fluid operation load and structural vibration excitation force,fatigue cracks initiated and continued to propagate at the defect location,ultimately leading to fatigue fracture of the guide vane.

王铭昌;李楠;车银辉;杨小虎;杨曦

国家核电厂安全及可靠性工程技术研究中心,苏州 215008||苏州热工研究院有限公司,苏州 215008国家核电厂安全及可靠性工程技术研究中心,苏州 215008||苏州热工研究院有限公司,苏州 215008国家核电厂安全及可靠性工程技术研究中心,苏州 215008||苏州热工研究院有限公司,苏州 215008国家核电厂安全及可靠性工程技术研究中心,苏州 215008||苏州热工研究院有限公司,苏州 215008国家核电厂安全及可靠性工程技术研究中心,苏州 215008||苏州热工研究院有限公司,苏州 215008

通用工业技术

辅助给水泵导叶疲劳断裂铸造缺陷应力集中

auxiliary feedwater pumpguide vanefatigue fracturecasting defectstress concentration