首页|期刊导航|福建冶金|铸坯缺陷对60Si2Mn圆钢热顶锻开裂影响的研究与分析

铸坯缺陷对60Si2Mn圆钢热顶锻开裂影响的研究与分析OA

Study and Analysis on the Impact of Billet Defects on Hot Upsetting Cracking of 60Si2Mn Round Steel

中文摘要英文摘要

针对某钢厂 60Si2Mn 圆钢热顶锻批量开裂问题,通过多种检测手段明确铸坯缺陷是核心诱因,包括有害元素超标、内部疏松缩孔、偏析、夹杂物及表面裂纹气泡等,并从铸坯质量角度系统分析了开裂机理及影响因素.通过强化设备精度、优化冶炼浇铸工艺、采用专用保护渣等措施,热顶锻合格率从 92.11%提升至98.09%,为同类弹簧钢质量控制提供参考.

Regarding the batch cracking issue of hot upset forged 60Si2Mn round steel in a certain steel plant,various inspection methods identified the core causes as casting defects,including excessive harmful elements,internal looseness and shrinkage cavities,segregation,inclusions,and surface cracks or bubbles.From the perspective of casting quality,the cracking mechanism and influencing factors were systematically analyzed.By enhancing equipment precision,optimizing smelting and casting processes,and employing specialized protective slag,the hot upset forging pass rate increased from 92.11%to 98.09%,providing a reference for quality control of similar spring steels.

夏帅

福建三钢闽光股份有限公司,福建 三明 365000

60Si2Mn圆钢铸坯缺陷热顶锻开裂工艺优化

60Si2Mn round steelingot defectshot upset crackingprocess optimization

《福建冶金》 2026 (5)

30-32,3

评论